說明:J427CrCu是低氫型耐候鋼焊條,采用直流反接,可進行全位置焊接,熔敷金屬具有優(yōu)良的耐大氣腐蝕性能,良好的塑性和韌性。
用途:用于焊接12MnCrCu等耐候鋼結構。
熔敷金屬化學成分(%)
|
C |
Mn |
Si |
S |
P |
Cr |
Cu |
保證值 |
≤ 0.12 |
0.30-0.70 |
≤ 0.35 |
≤0.035 |
≤0.040 |
0.30-0.80 |
0.20-0.50 |
例值 |
0.063 |
0.65 |
0.30 |
0.006 |
0.015 |
0.60 |
0.30 |
熔敷金屬力學性能
試驗項目 |
Rm (N/mm2) |
ReL/Rp0.2 (N/mm2) |
49.4000pt; padding: 0.0000pt 5.4000pt 0.0000pt 5.4000pt; mso-border-left-alt: 0.5000pt solid #000000; mso-border-right-alt: 0.5000pt solid #000000; mso-border-top-alt: 0.5000pt solid #000000; mso-border-bottom-alt: 0.5000pt solid #000000; border: 0.5000pt solid #000000;" rowspan="2" width="65" valign="center">
A (%) |
KV2(J) |
-20℃ |
||||
保證值 |
≥420 |
≥330 |
49.4000pt; padding: 0.0000pt 5.4000pt 0.0000pt 5.4000pt; border-left: 0.5000pt solid #000000; mso-border-left-alt: 0.5000pt solid #000000; border-right: 0.5000pt solid #000000; mso-border-right-alt: 0.5000pt solid #000000; border-top: none; mso-border-top-alt: 0.5000pt solid #000000; border-bottom: 0.5000pt solid #000000; mso-border-bottom-alt: 0.5000pt solid #000000;" width="65" valign="center">
≥22 |
≥27 |
例值 |
565 |
480 |
49.4000pt; padding: 0.0000pt 5.4000pt 0.0000pt 5.4000pt; border-left: 0.5000pt solid #000000; mso-border-left-alt: 0.5000pt solid #000000; border-right: 0.5000pt solid #000000; mso-border-right-alt: 0.5000pt solid #000000; border-top: none; mso-border-top-alt: 0.5000pt solid #000000; border-bottom: 0.5000pt solid #000000; mso-border-bottom-alt: 0.5000pt solid #000000;" width="65" valign="center">
27 |
153 |
藥皮含水量≤0.60%
X射線探傷要求:I級
焊接位置
參考電流(DC+)
焊條直徑(mm) |
Φ3.2 |
Φ4.0 |
Φ5.0 |
焊接電流(A) |
80-120 |
130-180 |
170-240 |
注意事項:
1. 焊前焊條須經350℃烘焙1小時,隨用隨烘。
2. 焊前必須清除焊件的鐵銹、油污、水份等雜質。